Oxyhydride

An oxyhydride is a mixed anion compound containing both oxide O2− and hydride ions H−. These compounds may be unexpected as the hydrogen and oxygen could be expected to react to form water. But if the metals making up the cations are electropositive enough, and the conditions are reducing enough, solid materials can be made that combine hydrogen and oxygen in the negative ion role.

Production

The first oxyhydride to be discovered was lanthanum oxyhydride, a 1982 discovery. It was made by heating lanthanum oxide in an atmosphere of hydrogen at 900 °C. However, heating transition metal oxides with hydrogen usually results in water and the reduced metal.

Topochemical synthesis retains the basic structure of the parent compound, and only does the minimum rearrangements of atoms to convert to the final product. Topotactic transitions retain the original crystal symmetry. Reactions at lower temperatures do not distort the existing structure. Oxyhydrides in a topochemical synthesis can be produced by heating oxides with sodium hydride NaH or calcium hydride CaH2 at temperatures from 200–600 °C. TiH2 or LiH can also be used as an agent to introduce hydride. If calcium hydroxide or sodium hydroxide is formed, it might be able to be washed away. However for some starting oxides, this kind of hydride reduction might just yield an oxygen-deficient oxide.

Reactions under hot high-pressure hydrogen can result from heating hydrides with oxides. A suitable seal for the lid on the container is required, and one such substance is sodium chloride.

Oxyhydrides all contain an alkali metal, alkaline earth metal, or rare-earth element, which are needed in order to put electronic charge on hydrogen.

Properties

The hydrogen bonding in oxyhydrides can be covalent, metallic, and ionic bonding, depending on the metals present in the compound.

Oxyhydrides lose their hydrogen less than the pure metal hydrides.

The hydrogen in oxyhydrides is much more exchangeable. For example oxynitrides can be made at much lower temperatures by heating the oxyhydride in ammonia or nitrogen gas (say around 400 °C rather than 900 °C required for an oxide) Acidic attack can replace the hydrogen, for example moderate heating in hydrogen fluoride yields compounds containing oxide, fluoride, and hydride ions (oxyfluorohydride.) The hydrogen is more thermolabile, and can be lost by heating yielding a reduced valence metal compound.

Changing the ratio of hydrogen and oxygen can modify electrical or magnetic properties. Then band gap can be altered. The hydride atom can be mobile in a compound undergoing electron coupled hydride transfer. The hydride ion is highly polarisable, so it presence raised the dielectric constant and refractive index.

Some oxyhydrides have photocatalytic capability. For example BaTiO2.5H0.5 can function as a catalyst for ammonia production from hydrogen and nitrogen.

The hydride ion is quite variable in size, ranging from 130 to 153 pm.

The hydride ion actually does not only have a −1 charge, but will have a charge dependent on its environment, so it is often written as Hδ−. In oxyhydrides, the hydride ion is much more compressible than the other atoms in compounds. Hydride is the only anion with no π orbital, so if it is incorporated into a compound, it acts as a π-blocker, reducing dimensionality of the solid.

Oxyhydride structures with heavy metals cannot be properly studied with X-ray diffraction, as hydrogen hardly has any effect on X-rays. Neutron diffraction can be used to observe hydrogen, but not if there are heavy neutron absorbers like Eu, Sm, Gd, Dy in the material.

List

Formula Structure Space group Unit cell Volume Density Comments Reference
Na3SO4H tetrahedral P4/nmm a=7.0034 c=4.8569
[η1-3,5-tBu2pz(η-Al)H)2O]2 pz=pyrazolato triclinic P1 a=10.202 b=13.128 c=13.612 α=112.39 β=101.90 γ=96.936 Z=1 1608.7 1.162
(MeLAlH)2(μ-O)

MeL = HC[(CMe)N(2,4,6-Me3C6H2)]2–

white
CaTiO3−xHx (x ≤ 0.6) Conducting; H in disordered position
Mg2AlNiXHZOY
Sr2LiH3O ionic conductor
Sr3AlO4H tetragonal I4/mcm a =6.7560 c =11.1568
Sr21Si2O5H14 cubic
Sr5(BO3)3H orthorhombic Pnma a=7.1982, b=14.1461, c=9.8215 1000.10 decomposed by water
LiSr2SiO4H monoclinic P21/m a = 6.5863, b = 5.4236, c = 6.9501, β = 112.5637 air stable
Sr21Si2O5H12+x cubic Fd3m a = 19.1190
Sr5(PO4)3H hexagonal P63/m a = 9.7169, c = 7.2747 594.83 for deuteride
Sr2CaAlO4H tetragonal I4/mcm a= 6.6220 c= 10.9812 481.531
SrScO2H cubic Pm3m a = 4.0483 mechanochemical synthesis
SrTiO3−xHx (x ≤ 0.6) Conducting; H in disordered position
SrVO2H
Sr2VO3H
Sr3V2O5H2
SrCrO2H cubic produced under 5GPa 1000 °C
Sr3Co2O4.33H0.84 insulator
YHO orthorhombic Pnma a = 7.5367, b = 3.7578, c = 5.3249
YOxHy photochromic; band gap 2.6 eV
Zr3V3OD5
Zr5Al3OH5
Ba3AlO4H orthorhombic Pnma Z=4,a=10.4911,b=8.1518,c=7.2399
Ba21Si2O5H14 cubic Fd3m a=20.336
Ba21Si2O5H24 cubic Fd3m a = 20.336 Zintl phase
BaScO2H cubic Pm3m a=4.1518
Ba2ScHO3 H− conductor
BaTiO3−xHx (x ≤ 0.6) Conducting; H in disordered position
Ba2NaTiO3H3 cubic Fm3m a=8.29714
BaVO3−xHx (x = .3) 5 GPa hexagonal, 7GPa cubic
Ba2NaVO2.4H3.6 cubic Fm3m a=8.22670
BaCrO2H hexagonal P63/mmc a =5.6559 c =13.7707
Ba2NaCrO2.2H3.8 cubic Fm3m a=8.17470
Ba21Zn2O5H12 cubic Fd3m a = 20.417
Ba21Zn2O5H24 cubic Fd3m a = 20.417
Ba21Ga2O5H24 cubic Fd3m Zintl phase
Ba21Ge2O5H14 cubic Fd3m a=20.356
Ba21Ge2O5H24 cubic Fd3m a = 20.356 Zintl phase
Ba21As2O5H16 cubic Fd3m a=20.230
Ba21As2O5H24 cubic Fd3m a = 20.230
Sr2BaAlO4H tetragonal I4/mcm a =6.9093 c =11.2107
BaYO2H cubic Pm3m a = 4.3068 mechanochemical synthesis
Ba2YHO3 a=4.38035 c=13.8234 H− conductor
Ba21Cd2O5H12 cubic Fd3m a=20.633
Ba21Cd2O5H24 cubic Fd3m a = 20.633
Ba21In2O5H12 cubic Fd3m a=20.607
Ba21In2O5H24 cubic Fd3m a = 20.607 Zintl phase
Ba21Sn2O5H14 cubic Fd3m a=20.532
Ba21Sn2O5H24 cubic Fd3m a = 20.532
Ba21Sb2O5H16 cubic Fd3m a=20.419
Ba21Sb2O5H24 cubic Fd3m a = 20.419
Ba21Pb2O5H14 cubic Fd3m a=20.597
LaHO
La2LiHO3 orthorhombic Immm a=3.57152 b=3.76353 c=12.9785
La0.6Sr1.4LiH1.6O2 H− conductor
LaSr3NiRuO4H4
LaSrMnO3.3H0.7 high-pressure fabrication
LaSrCoO3H0.7 insulator
CeHO
CeNiHZOY Catalyse ethanol to H2
Nd0.8Sr0.2NiO2Hx (x = 0.2–0.5) superconductor for x between 0.22 and 0.28
NdHO P4/nmm

P62m

a=7.8480, c=5.5601 V=342.46

a = 5.99429, c = 3.49252

3 GPa
PrHO
GdHO Fm3m

P62m

a = 5.38450

a = 5.84710, c = 3.38983

5 GPa
EuTiO3−xHx (x ≤ 0.6) Conducting; H in disordered position
HoHO F43m a = 5.2755 light-yellow under the sun; pink indoors
DyHO cubic F43m a=5.3095
ErHO cubic F43m

P62m

a=5.24615

a = 5.70986, c = 3.29915

5 GPa
LuHO cubic F43m a=5.17159
LuHO orthorhombic Pnma a = 7.3493, b = 3.6747, c = 5.1985
Ba21Hg2O5H12 cubic Fd3m a=20.507
Ba21Tl2O5H12 cubic Fd3m a=20.68
Ba21Tl2O5H24 cubic Fd3m a = 20.68 Zintl phase
Ba21Hg2O5H24 cubic Fd3m a = 20.507
Ba21Pb2O5H24 cubic Fd3m a = 20.597
Ba21Bi2O5H16 cubic Fd3m a=20.459
PuHO Formed during corrosion of plutonium metal in water

Three or more anions

Formula Structure Space group Unit cell Comments Reference
Eu2LiHOCl2 orthorhombic Cmcm a = 14.923 b = 5.7012 c = 11.4371 Z = 8 density 5.444; yellow
Sr2LiHOCl2 orthorhombic Cmcm a = 15.0235 b = 5.69899 c = 11.4501 synthesized at ambient pressure and 2 GPa; ordered H/O
Sr2LiHOCl2 tetragonal I4/mmm a = 4.04215 c = 15.04359 synthesized at 5 GPa; disordered H/O
Sr2LiHOBr2 tetragonal I4/mmm a = 4.1097 c = 16.1864 synthesized at 5 GPa; disordered H/O
Ba2LiHOCl2 tetragonal I4/mmm a = 4.26816 c = 15.6877 synthesized at 5 GPa; disordered H/O